test               eta start  eta end  average  fracture
shear                  0.030    0.080    0.055     0.510
dogbone                0.333    0.450    0.380     0.519
notch R5               0.400    0.500    0.467     0.452
plane strain R2        0.530    0.570    0.559     0.368
Nakajima biaxial       0.640    0.665    0.658     0.503

Failure curve: hosford_coulomb a 1.467, b 0.5906, c 0.03169, n 0.1
test                   eta  measured predicted   error
shear                0.055    0.5100    0.5099   -0.0%
dogbone              0.380    0.5190    0.5305    2.2%
notch R5             0.467    0.4520    0.4378   -3.1%
plane strain R2      0.559    0.3680    0.3773    2.5%
Nakajima biaxial     0.658    0.5030    0.4940   -1.8%

Failure curve: johnson_cook d1 0.4119, d2 0.1162, d3 -1.955
test                   eta  measured predicted   error
shear                0.055    0.5100    0.5161    1.2%
dogbone              0.380    0.5190    0.4680   -9.8%
notch R5             0.467    0.4520    0.4586    1.5%
plane strain R2      0.559    0.3680    0.4507   22.5%
Nakajima biaxial     0.658    0.5030    0.4441  -11.7%

failure strain      eta      HC      JC   truth
compression      -0.333   1.113   0.635   1.093
shear             0.000   0.528   0.528   0.516
uniaxial          0.333   0.591   0.472   0.600
plane strain      0.577   0.374   0.449   0.372
equibiaxial       0.667   0.591   0.443   0.600
(compression is extrapolated: no test below shear)

ECRIT from the FLC (triaxiality, critical strain):
  (-0.333, 0.361)  (0.296, 0.361)  (0.363, 0.220)  (0.577, 0.162)  (0.653, 0.255)  (0.664, 0.362)  (0.667, 0.362)

LCREGD estimate: 0.5 mm 1.000, 1 mm 1.000, 2.5 mm 0.522, 5 mm 0.363, 10 mm 0.283

Card check: 0 errors, 1 warnings
  warning: from element size 2.5 mm the regularised failure strain is at or below the critical strain (triaxiality -0.16 to 0.32, 0.613 to 0.64, 0.66 to 0.667): no fading there
2.5 mm shell, uniaxial: failure strain 0.308 (x 0.522), coupling at 0.282, D_crit 0.839
  strain       D       F  stress
   0.100   0.105   0.125  100.0%
   0.200   0.421   0.502  100.0%
   0.270   0.767   0.914  100.0%
   0.285   0.855   1.000   99.9%
   0.295   0.916   1.000   89.1%
   0.300   0.947   1.000   69.7%
   0.305   0.979   1.000   34.2%
   0.310   1.000   1.000    0.0%

*MAT_ADD_DAMAGE_GISSMO
$#     mid      dtyp     refsz    numfip
       800       1.0       0.0       1.0
$#   lcsdg     ecrit    dmgexp     dcrit    fadexp    lcregd
      2800   -2900.0       2.0       0.0       3.0      3000
$#   lcsrs      shrf     biaxf
         0       0.0       0.0
*DEFINE_CURVE_TITLE
GISSMO 800 failure strain vs triaxiality
$#    lcid      sidr       sfa       sfo      offa      offo
      2800         0       1.0       1.0       0.0       0.0
$#                a1                  o1
         -0.66666667            1.113432
         -0.63333333          0.81831472
...
MID 800 (mm-ms-kg): passed
  warning: from element size 2.5 mm the regularised failure strain is at or below the critical strain (triaxiality -0.16 to 0.32, 0.613 to 0.64, 0.66 to 0.667): no fading there
Read back: 4 curves; failure strain equal to 1e-6: yes